Getting Gold: A Gold-Mining Handbook for Practical Men
The Frue vanner will, as a rule, act well when the pulp is sufficiently and consistently fine. It is an adaptation of the old simple apparatus used in China and India for washing gold dust from river sand. The original consisted of an endless band of strong cloth or closely woven matting, run on two horizontal rollers placed about seven feet apart, one being some inches lower than the other. The upper is caused to revolve by means of a handle. The cloth is thus dragged upwards against a small stream of water and sand fed to it by a second man, the first man not only turning the handle but giving a lateral motion to the band by means of a rope tied to one side.
Chinamen were working these forerunners of the Frue vanner fifty years ago in Australia, and getting fair returns.
The Frue vanner (Fig. 24) is an endless india-rubber band drawn over an inclined table, to which a revolving and side motion is given by ingenious mechanism, the pulp being automatically fed from the upper end, and the concentrates collected in a trough containing water in which the band is immersed in its passage under the table; the lighter particles wash over the lower end. The only faults with the vanner are—first, it is rather slow; and secondly, though so ingenious it is just a little complicated in construction for the average non-scientific operative.
Of pan concentrators there is an enormous selection, the principle in most being similar—i.e., a revolving muller, which triturates the sand, so freeing the tiny golden particles and admitting of their contact with the mercury. The mistake with respect to most of these machines is the attempt to grind and amalgamate in one operation. Even when the stone under treatment contains no deleterious compounds the simple action of grinding the hard siliceous particles has a bad effect on the quicksilver, causing it to separate into small globules, which either oxidising or becoming coated with the impurities contained in the ore will not reunite, but wash away in the slimes and take with them a percentage of the gold. As a grinder and concentrator, and in some cases as an amalgamator, when used exclusively for either purpose, the Watson and Denny pan (Fig. 25) is effective; but although successfully used at one mine I know, the mode there adopted would, for reasons previously given, be very wasteful in many other mines.
There is much misconception, even among men with some practical knowledge, as to the proper function of these saving appliances; and sometimes good machines are condemned because they fail to perform work they were not intended for.
It cannot be too clearly realised that the correct order of procedure for extracting the gold held in combination with base metals is—first, reduction of the particles to a uniform gauge and careful concentration only; next, the dissipation, usually by simple calcination, of substances in the concentrates inimical to the thorough absorption of the gold by the mercury; and lastly, the amalgamation of the gold and mercury.
For general purposes, where the gangue has not been crushed too fine, I think the Duncan pan will usually be found effective in saving the concentrates. In theory it is an enlargement of the alluvial miner’s tin dish, and the motion imparted to it is similar to the eccentric motion of that simple separator.
The calcining may be effectively carried out in an ordinary reverberatory furnace, the only skill required being to prevent over “roasting” and so slagging the concentrates; or not sufficiently calcining so as to remove all deleterious constituents; the subject, however, is fully treated in Chapter VIII.
For amalgamating I prefer some form of settler to any further grinding appliance, but I note also improvements in the rotary amalgamating barrel, which, though slow, is, under favourable conditions, an effective amalgamator. The introduction of steam under pressure into an iron cylinder containing a charge of concentrates with mercury is said to have produced good results, and I am quite prepared to believe such would be the case, as we have long known that the application of steam to ores in course of amalgamation facilitates the process considerably.
Some twenty-five years since I also was engaged on the construction of a dry amalgamator in which sublimated mercury was passed from a retort through the descending gangue in a vertical cylinder, the material falling therefrom through an aperture into a revolving settler, the object being to save water on mines in dry country. The model, about quarter size, was completed, when my attention was called to an American invention, in which the same result was stated to be attained more effectively by blowing the mercury spray through the triturated material by means of a steam jet. I had already encountered a difficulty, since found so obstructive by experimentalists in the same direction, that is, the getting of the mercury back into its liquid metallic form. This difficulty can be largely obviated by my own device of using a very weak solution of sulphuric acid (it can hardly be too weak) and adding a small quantity of zinc to the mercury. It is perfectly marvellous how some samples of mercury “sickened” or “floured” by bad treatment, may be brought back to the bright, clean, easy flowing metal by a judicious use of these inexpensive materials.
Thus it will probably be found practicable to crush dry and amalgamate semi-dry by passing the material in the form of a thin pasty mass to a settler, as in the old South American arrastra, and, by slowly stirring, recover the mercury, and with it the bulk of the gold.
The following is from the Australian Mining Standard, and was headed “Amalgamation Without Overflow”:
“Recent experiments at the Ballarat School of Mines have proved that a deliverance from difficulties is at hand from an unexpected quarter. The despised Chilian mill and Wheeler pan, discarded at many mines, will solve the problem, but the keynote of success is amalgamation without overflow. Dispense with the overflow and the gold is saved.
“Two typical mines—the Great Mercury Proprietary Gold Mine, of Kuaotunu, N.Z., the other, the Pambula, N.S.W.—have lately been conducting a series of experiments with the object of saving their fine gold in an economical manner. The last and best trials made by these companies were at the Ballarat School of Mines, where amalgamation without overflow was put to a crucial test, in each case with the gratifying result that ninety-six per cent. of the precious metal was secured. What this means to the Great Mercury Mine, for instance, can easily be imagined when it is understood that notwithstanding all the latest gold-saving adjuncts during the last six months 1260 tons of ore, worth £4. 17s. 10⅔d. a ton, have been put through for a saving of £1 9s. 1⅔d. only; or in other words over two-thirds of the gold has gone to waste (for the time being) in the tailings, and in the tailings at the present moment lie the dividends that should have cheered shareholders’ hearts.
“And now for the modus operandi, which, it must be remembered, is not hedged in by big royalties to any one, rights, patent or otherwise. The ore to be treated is first calcined, then put through a rock-breaker or stamper battery in a perfectly dry state. If the battery is used, ordinary precautions, of course, must be taken to prevent waste, or the dust becoming obnoxious to the workmen. The ore is then transferred to the Chilian mill and made to the consistency of porridge, the quicksilver being added. When the principal work of amalgamation is done (experience soon teaching the amount of grinding necessary), from the Chilian mill the paste (so to say) is passed to a Wheeler or any other good pan of a similar type, when the gold-saving operation is completed.”
This being an experiment in the same direction as my own, I tried it on a small scale. I calcined some very troublesome ore till it was fairly “sweet,” triturated it, and having reduced it with water to about the consistency of invalid’s gruel, put it into a little berdan pan made from a “camp oven,” which I had used for treating small quantities of concentrates, and from time to time drove a spray of mercury, wherein a small amount of zinc had been dissolved, into the pasty mass by means of a steam jet, added about half an ounce of sulphuric acid and kept the pan revolving for several hours. The result was an unusually successful amalgamation and consequent extraction—over ninety per cent.
Steam—or to use the scientific term, hydro-thermal action—has played such an important part in the deposition of metals that I cannot but think that under educated intelligence it will prove a powerful agent in their extraction. Twenty-five years ago I obtained some rather remarkable results from simply boiling auriferous ferro-sulphides in water. There is in this alone an interesting, useful, and profitable field for investigation and experiment.
The most scientific and perfect mode of gold extraction (when the conditions are favourable) is lixiviation by means of chlorine, potassium cyanide, or other aurous solvent, for by this means as much as 98 per cent. of the gold contained in suitable ores can be converted into its mineral salt, and being dissolved in water, re-deposited in metallic form for smelting; but lode stuff containing much lime would not be suitable for chlorination, or the presence of a considerable proportion of such a metal as copper, particularly in metallic form, would be fatal to success, while cyanide of potassium will also attack metals other than gold, and hence discount the effect of that solvent.
The earlier practical applications of chlorine to gold extraction were known as Mears’ and Plattner’s processes, and consisted in placing the material to be operated on in vats with water, and introducing chlorine gas at the bottom, the mixture being allowed to stand for a number of hours, the minimum about twelve, the maximum forty-eight. The chlorinated water was then drawn off containing the gold in solution which was deposited as a brown powder by the addition of sulphate of iron.
Great improvements on this slow and imperfect method have been made of late years, among the earlier of which was that of Messrs. Newbery and Vautin. They placed the pulp with water in a gas-tight revolving cylinder, into which the chlorine was introduced, and atmospheric air to a pressure of 60 lb. to the square inch was pumped in. The cylinder with its contents was revolved for two hours, then the charge was withdrawn and drained nearly dry by suction, the resultant liquid being slowly filtered through broken charcoal on which the chloride crystals were deposited, in appearance much like the bromo-chlorides of silver ore seen on some of the black manganic oxides of the Barrier silver mines. The charcoal, with its adhering chlorides, was conveyed to the smelting-house and the gold smelted into bars of extremely pure metal. Messrs. Newbery and Vautin claimed for their process decreased time for the operation with increased efficiency.
At Mount Morgan, when I visited that mine in the eighties, they were using what might be termed a composite adaptation process. Their chlorination works, the largest in the world, were putting through 1500 tons per week. The ore as it came from the mine was fed automatically into Krumm roller mills, and after being crushed and sifted to regulation gauge was delivered into trucks and conveyed to the roasting furnaces, and thence to cooling floors, from which it was conveyed to the chlorinating shed. Here were long rows of revolving barrels, on the Newbery-Vautin principle, but with this marked difference, that the pressure in the barrel was obtained from an excess of the gas itself, generated from a charge of chloride of lime and sulphuric acid. On leaving the barrels the pulp ran into settling vats, somewhat on the Plattner plan, and the clear liquid having been drained off was passed through a charcoal filter, as adopted by Newbery and Vautin. The manager, Mr. Wesley Hall, stated that the estimated cost per ton was not more than 30s., and he expected shortly to reduce that when he began making his own sulphuric acid. As he was obtaining over 4 oz. to the ton the process was paying very well, but it will be seen that the price would be prohibitive for poor ores unless they could be concentrated before calcination.