In a stamp mill (Fig. 20) the foundations are usually made of hard-wood logs about 5 to 6 feet long, set on end, the bottom end resting on rock and set round with cement concrete. These are bolted together, and the “box” or mortar is bolted to them. The horizontal logs to carry the “horses” or supports for the battery frame should also be of good size, and solidly and securely bolted. The same applies to your engine bed, but whether it be of timber, or mason work, above all things provide that the whole of your work is set out square and true to save after wear and friction. Fig. 21 represents a 10-head stamp mill.

My experience has been that the most effective weight for stamps and height for drop largely depends on the nature of the rock foundation. I have usually found that with medium stamps, say 7½ to 8 cwt. with fair drop and lively action, about 80 falls per minute, the best results were obtained, but the tendency of modern mill men is towards the heavier stamps, 10 cwt. and even heavier.

Great improvements have been made in stamp mills since the sixteenth century, as is evident by comparing Fig. 21A with Figs. 20 and 21; even in the writer’s time they have been considerable.

To find the horse power required to drive a battery, multiply the weight of one stamp by the number of stamps in the battery; the height of lift in feet by the number of lifts per minute; add one-third of the product for friction, and the result will be the number of feet-lbs. per minute; divide this by 33,000 which is the number of feet-lbs. per minute equal to 1 h.-p. and the result will be the h.-p. required. Thus if a stamp weighs 800 lbs. and you have five in the box, and each stamp has a lift of 9 in. = 0·75 ft. and strikes 80 blows per minute, then ÷ 800 × 5 × 0·75 × 80 = 240,000; one third of 240,000 = 80,000, which added to 240,000 = 320,000; and 320,000 divided by 33,000 = 9·7 h.-p. or 1·9 h.-p. each stamp.

Fig. 20. Stamp Mill, showing Part of Foundations.
Fig. 21. 10-Head Stamp Mill.

The total weight of a battery, including stamper box, stampers, &c., may be roughly estimated at about 1 ton per stamp. Medium weight stampers, including shank, cam, disc, head, and shoe, weigh from 600-700 lbs., and need about ¾ h.-p. to work them.

Fig. 21a. Sixteenth Century Stamp Mill.

The quantity of water required for the effective treatment of gold bearing rock in a stamper battery varies according to the composition of the material to be operated upon, but generally it is more than the inexperienced believe. For instance, “mullocky” lode stuff, containing much clayey matter or material carrying a large percentage of heavy metal, such as titanic iron or metallic sulphides, will need a larger quantity of water per stamp than clean quartz. A fair average quantity would be 750 to 1000 gallons per hour for each box of five stamps. In general practice I have seldom found 1000 gallons per hour more than sufficient.

As to the most effective mesh for the screen or grating, that depends largely on the size of the gold particles contained in the gangue. The finer the particles the closer must be the mesh, so that nothing but careful experiment will enable the battery manager to decide this most important point. The American slotted screens are best; they wear better than the punched gratings and can be used of finer gauge. Woven steel wire gauze is employed with good effect in some mills where specially fine trituration is required. This class of screen requires special care as it is somewhat fragile, but with intelligent treatment does good work.

The fall or inclination of the tables, both copper and blanket strakes, is also regulated by the class of ore. If it should be heavy then the fall must be steeper. A fair average drop is ¾ inch to the foot. Be careful that your copper tables are thoroughly water-tight, for, remember, where water will percolate, mercury will penetrate.

The blanket tables are simply a continuation of the mercury tables, but covered with strips of coarse blanket, green baize, or other flocculent material, intended to arrest the heavier metallic particles which have not been amalgamated.

The blanket table is, however, a very unsatisfactory concentrator at best, and is giving place to mechanical concentrators of various descriptions.

I have a device at present unpatented which will do away with the necessity for blanket tables or copper plates, as by the expenditure of from ½ to 1 h.-p. every particle of free gold after leaving the boxes must come within the embrace of a mercury amalgam. No cleaning of plates is required.

An ancient Egyptian gold washing table is shown in Fig. 22. It is a representation of an old stone table such as is referred to in p. 2, which was used by the Egyptians in treating the gold ores of Lower Egypt. The ore was first ground, it is likely by means of some description of stone arrastra, and then passed over the sloping table with water, the gold being retained in the riffles. In these the material would probably be mechanically agitated. Although for its era ingenious it will be plain to practical men that if the gold were fine the process would be very ineffective. Possibly, but of this I have no evidence, mercury was used to retain the gold in the riffles, for, as previously stated, this method was known to the ancients.

Fig 22. Washing Table of Stone with Riffles.

At a mine at which I was managing director the lode was almost entirely composed of sulphide of iron, carbonate of lime or calcspar, with a little silica. In this case it was found best to crush without mercury, then run the pulp into pans, where it was concentrated. The concentrates were calcined in a common reverberatory furnace, and afterwards amalgamated with mercury in a special pan; the results were very satisfactory; but it does not follow that this process would be the most suitable for a slightly different lode stuff.

I was lately consulted with respect to the treatment of a pyritic ore in a very promising mine, but could not recommend the above treatment, because though the pyrites in the gangue was similar, the bulk of the lode consisted of silica, consequently there would be a great waste of power in triturating the whole of the stuff to what, with regard to much of it, would be an unnecessary degree of fineness. I am of opinion that in cases such as this, where it is not intended to adopt the chlorination or cyanogen process, it will be found most economical to crush to a coarse gauge, concentrate, calcine the concentrates, and finally amalgamate in some suitable amalgamator.

Probably for this mode of treatment Krom rolls would be found more effective reducing agents than stampers, as with them the bulk of the ore can be broken to any required gauge and there would consequently be less loss in “slimes.”

The great art in effective battery work is to crush your stuff to the required fineness only, and then to provide that each particle is brought into contact with the mercury either in box, trough plate, or pan. To do this the flow of water must be carefully regulated; it should not carry the stuff off too quickly nor allow the troughs and plates to be choked. In cold weather the water may be warmed by passing the feed-pipe through a tank into which the steam from the engine exhausts, and this will be found to keep the mercury bright and lively. But be careful no engine oil or grease mingles with the water, as grease on the copper tables will absolutely prevent amalgamation.

The first point, then, is to effectively crush the gangue, the degree of fineness being regulated by the fineness of the gold itself. This being done, then comes the question of saving the gold. If the quartz be clean, and the gold unmixed with base metal, the difficulty is small. All that is required is to ensure that each particle of gold shall be taken up by the mercury. The main object is to arrest the gold at the earliest possible stage; therefore, if you are treating clean stone containing free gold, either coarse or fine, I advise the use of mercury in the boxes, for the reason that a considerable proportion of the gold will be caught thereby, and settling to the bottom, or adhering to amalgamated plates in the boxes, where such are used, will not be afterwards affected by the crushing action, which might otherwise break up, or “flour,” the mercury. On the whole, I rather favour the use of mercury in the box at any time, unless the ore is very refractory—that is, contains too great a proportion of base metals, particularly sulphides of iron, arsenic, &c., when the result will not be satisfactory, but may entail great loss by the escape of floured mercury carrying with it particles of gold. Intelligent experience will assist the battery manager to adopt the right system.

The crushed stuff—generally termed the “pulp”—passes from the boxes through the “screens” or “gratings,” and so on to the “tables”—i.e., sheets of copper amalgamated on the upper surface with mercury, and sometimes electroplated with silver and afterwards treated with mercury. Unless the quartz is very clean, and, consequently light, I am opposed to the form of stamper box with mercury troughs cast in the “lip,” nor do I think that a trough under the lip is a good arrangement, as it usually gets so choked and covered with the heavy clinging base metals as to make it almost impossible for the gold to come in contact with the mercury. It will be found better where the gold is fine, or the gangue contains much base metal, to run the pulp from the lip of the battery into a “distributor.”

The distributor is a wooden box the full width of the stamper box or mortar, having a perforated iron bottom set some three to four inches above the first copper plate, which should come up under the lip. The effect of this arrangement is that the pulp is dashed on to the plate by the falling water, and the gold at once coming in contact with the mercury begins to accumulate and attract that which follows, till the amalgam becomes piled in little crater-shaped mounds, and thus 75 per cent. of the gold is saved on the top plate.

I have tried a further adaptation of this process when treating ores containing a large percentage of iron oxide, where the bulk of the gold is impalpably fine, and contained in the “gossan.” At the end of the blanket table, or at any point where the crushed stuff last passes before going to the “tailings heap” or “sludge pit,” a “saver” is placed. The saver is a strong box about 15 in. square by 3 ft. high, one side of which is removable, but must fit tight. Nine slots are cut inside at 4 in. apart, and into these are fitted nine square perforated copper plates, having about eighty to a hundred ¼ in. holes in each; the perforations should not come opposite each other. These plates are to be amalgamated on both sides with mercury, and the top plate “fed” from time to time with mercury, in which a very little sodium has been placed. If acid ores are being treated, zinc should be employed in place of sodium, and to prevent the plates becoming bare, if the stuff is very poor, thick zinc amalgam may be used with good effect; but in that case discontinue the sodium, and occasionally, if required, say once or twice in the day, mix an ounce of sulphuric acid in a half gallon of water and slowly pour it into the launder above the saver. Underneath the “saver” you require a few riffles, or troughs, to catch any waste mercury, but if not overfed there should be no waste. This automatic appliance sometimes arrests a considerable quantity of gold.