Getting Gold: A Gold-Mining Handbook for Practical Men
We now come to the subsidiary processes of battery work, the “cleaning” of plates, and “scaling” same when it is desired to get all the gold off them, the cleaning and retorting of amalgam, and of the mercury, smelting gold, &c.
Plates should be tenderly treated, kept as smooth as possible, and when cleaning up after crushing, in your own battery, the amalgam—except, say, at half-yearly intervals—should be removed with a rubber only; the rubber is simply a square of black india-rubber or soft pine wood.
When crushing rich ore, and you want to get nearly all the gold off your plates, the scraper (Fig. 23) may be resorted to. This is usually made by the mine blacksmith from an old flat file which is cut in half, the top turned over, beaten out to a sharp blade, and kept sharp by touching it up on the grinding-stone. This, if carefully used, will remove the bulk of the amalgam without injury to the plate.
Various methods of “scaling” plates will be found among “Rules of Thumb.”
Where base metals are present in the lode stuff frequent retortings of the mercury, say not less than once a month, will be found to have a good effect in keeping it pure and active. For this purpose, and in order to prevent stoppage of the machinery, a double quantity is necessary, so that half may be used alternately. Less care is required in retorting the mercury than in treating the amalgam, as the object in the one case is more to cleanse the metal of impurities than to save gold, which will for the most part have been extracted by squeezing through the chamois leather or calico. A good strong heat may therefore at once be applied to the retort and continued, the effect being to oxidise the arsenic, antimony, lead, &c., which, in the form of oxides, will not again amalgamate with the mercury, but will either lie on its surface under the water, into which the nozzle of the retort is inserted, or will float away on the surface of the water. I have also found that covering the top of the mercury with a few inches of broken charcoal when retorting has an excellent purifying effect.
In retorting amalgam, much care and attention is required.
First, never fill the retort too full, give plenty of room for expansion; for, when the heat is applied, the amalgam will rise like dough in an oven, and may be forced into the discharge pipe, the consequence being a loss of amalgam or the possible bursting of the retort. Next, be careful in applying the heat, which should be done gradually, commencing at the top. This is essential to prevent waste and to turn out a good-looking cake of gold, which all battery managers like to do, even if they purpose smelting into bars.
Sometimes special difficulties crop up in the process of separating the gold from the amalgam. At the first “cleaning up” on the Frasers Mine at Southern Cross, West Australia, great consternation was excited by the appearance of the retorted gold, which, as an old miner graphically put it, was “as black as the hind leg of a crow,” and utterly unfit for smelting, owing to the presence of base metals. Some time after this I was largely interested in the Blackborne mine in the same district when a similar trouble arose. This I succeeded in surmounting, but a still more serious one was too much for me—i.e., the absence of payable gold in the stone. I give here an extract from the Australian Mining Standard, of December 9th, 1893, with reference to the mode of cleaning the amalgam which I adopted.
NEW METHOD OF SEPARATING GOLD FROM IMPURE AMALGAM.
I had submitted to me lately a sample of amalgam from a mine in West Australia which amalgam had proved a complete puzzle to the manager and amalgamator. The Mint returns showed a very large proportion of impurity, even in the smelted gold. When retorted only, the Mint authorities refused to take it after they had treated the first two cakes, one of 119 oz., which yielded only 35 oz. 5 dwt. standard gold, and one of 140 oz., which gave 41 oz. 10 dwt. The gold smelted on the mine was nearly as bad proportionately. Thus, 128 oz. smelted down at the Mint to 87 oz. 8 dwt. and 109 oz. to 55 oz. 10 dwt. The impurity was principally iron, a most unusual thing in my experience, and was due to two causes revealed by assay of the ore and analysis of the mine water, viz., an excess of arsenate of iron in the stone, and the presence in large proportions of mineral salts, principally chloride of calcium CaCl₂, sodium NaCl, and magnesium MgCl₂, in the mine water used in the battery. The exact analysis of the water was as follows:—
| Carbonate of Iron | FeCO₃ | 2·76 | grains per gallon |
| Carbonate of Calcium | CaCO₃ | 7·61 | ” ” |
| Sulphate of Calcium | CaSO₄ | 81·71 | ” ” |
| Chloride of Calcium | CaCl₂ | 2797·84 | ” ” |
| Chloride of Magnesium | MgCl₂ | 610·13 | ” ” |
| Chloride of Sodium or Common Salt | NaCl | 5072·65 | ” ” |
| —— | |||
| Total solid matter | 8572·70 | = 19·5 oz. to the gallon |
It will be seen, then, that this water is nearly four times more salt than that of the sea. The effect of using a water of this character, as I have previously found, is to cause the amalgamation of considerable quantities of iron with the gold as in this case.
I received 10 oz. of amalgam, and having found what constituted its impurities proceeded to experiment as to its treatment. When retorted on the mine it was turned out in a black cake so impure as almost to make it impossible to smelt properly. I found the same result on first retorting, and after a number of experiments which need not be recapitulated, though some were fairly effective, I hit on the following method, which proved to be most successful and will probably be so found in other localities where similarly unfavourable conditions prevail.
I took a small ball of amalgam, placed it in a double fold of new fine-grained calico, and after soaking in hot water put it under a powerful press. The weight of the ball before pressing was 1583 gr. From this 383 gr. of mercury were expressed and five-eighths of a grain of gold was retorted from this expressed mercury. The residue, in the form of a dark, grey, and very friable cake, was powdered up between the fingers and retorted, when it became a brown powder; it was afterwards calcined on a flat sheet in the open air; result, 510 gr. of russet-coloured powder. Smelted with borax, the iron oxide readily separated with the slag; result, 311 gr. gold 871-1000 fine; a second smelting brought this up to 914-1000 fine. Proportion of smelted gold to amalgam, one-fifth.
The principal point about this mode of treatment is the squeezing out of the mercury, whereby the amalgam goes into the retort in the form of powder, thus preventing the slagging of the iron and enclosure of the gold. The second point of importance is thorough calcining before smelting.
Of course it would be practicable, if desired, to treat the powder with hydrochloric acid, and thus remove all the iron, but in a large way this would be too expensive, and my laboratory treatment, though necessarily on a small scale, was intended to be on a practical basis.
The amalgam at this mine was in this way afterwards treated with great success.
For the information of readers who do not understand the chemical symbols it may be said that
| FeCO₃ | is carbonate of iron; |
| CaCO₃ | is carbonate of calcium; |
| CaSO₄ | is sulphate of calcium; |
| CaCl₂ | is chloride of calcium; |
| MgCl₂ | is chloride of magnesium; |
| NaCl | is chloride of sodium, or common salt |
CHAPTER VII
GOLD EXTRACTION—SECONDARY PROCESSES AND LIXIVIATION
Before any plan is adopted for treating the ore in a new mine the management should very seriously and carefully consider the whole circumstances of the case, taking into account the quantity and quality of the lode stuff to be operated on, and ascertain by analysis what are its component parts, for, as before stated, the treatment which will yield most satisfactory results with a certain class of gangue on one mine will sometimes, even when the material is apparently similar, prove a disastrous failure in another. Some time since I was glad to note that the manager of what has since become a very prominent Australian mine strongly discountenanced the purchase of any extracting plant until he was fully satisfied as to the character of the bulk of the ore he would have to treat. It would be well for the pockets of shareholders and the reputation of managers if more of our mine superintendents followed this prudent and sensible course.
Having treated on gold extraction with mercury by amalgamated plates and their accessories, something must be said about secondary modes of saving in connection with the amalgamation process. The operations described hitherto have been the disintegration of the gold-bearing material and the extraction therefrom of the coarser free gold. But it must be understood that most auriferous lode stuff contains a proportion of sulphides of various metals, wherein a part of the gold, usually in a very finely divided state, is enclosed, and on this gold the mercury has no influence. Also many lodes contain hard heavy ferric ores, such as titanic iron, tungstate of iron, and hematite, in which gold is held. In others, again, are found considerable quantities of soft powdery iron oxide or “gossan,” and compounds such as limonite, aluminous clay, &c., which, under the action of the crushing mill become finely divided and float off in the water as “slimes,” carrying with them atoms of gold, often microscopically small. To save the gold in such matrixes as these is an operation which even the best of our mechanical appliances have not yet fully accomplished.
Where there is not too great a proportion of base metals on which the solvent will act, and when the material is rich enough in gold to pay for the extra cost of treatment, chlorination or cyanisation are the best modes of extraction yet practically adopted.
Presuming, however, that we are working by the amalgamation process, and have crushed our stone and obtained the free gold, the next requirement is an effective concentrator to secure the heavy base metals which hold a percentage of gold. There are many, and some do excellent work, but do not act equally well in all circumstances. The first and most primitive is the blanket table (p. 79); but it can hardly be said to be very effective, and requires constant attention and frequent changing and washing of the strips of blanket.
Instead of blanket tables percussion tables are sometimes used, to which a jerking motion is given against the flow of the water and pulp, and by this means the heavier minerals are gathered towards the upper part of the table, and are removed when concentrated. I have seen this appliance doing fairly good work, but it is by no means a perfect concentrator.
Another form of “shaking table” is one with a lateral motion, and this, whether with amalgamated plates, or provided with small riffles, or covered with blanket, keeps the pulp lively and encourages the retention of the heavier particles, whether of gold or base metals containing gold. There has also been devised a rocking table, the action of which is analogous to that of the ordinary miner’s cradle. This appliance, working somewhat slowly, swings on rockers from side to side, and is usually employed in mills where, owing to the complexity of the ore, difficulties have been met with in amalgamating the gold. Riffles are provided and even very fine gold is sometimes effectively recovered by their aid.