Getting Gold: A Gold-Mining Handbook for Practical Men
I have had no experience with the aluminium bronze screen. I presume, however, that it is used only for mills where mercury is not put in the mortars, otherwise it would surely become amalgamated. The same remark applies to brass wire cloth and tinned plate. Unless the metal of which they are composed will not readily amalgamate with mercury, I should be chary of using new screen devices. Mercury is a most insidious metal and is often found most unexpectedly in places in the battery where it should not be. Probably aluminium steel would be better than any substance mentioned. It would be hard, light, strong, and not readily corrodible. I am not aware if it has been tried.
Under the heading of “Power for Mills” the following is taken from the same source.
POWER FOR MILLS.
“As the Pelton wheel seems to find the most frequent application in California, it may be convenient for millmen to have the following rule, applicable to these wheels:
“When the head of water is known in feet, multiply it by 0·0024147, and the product is the horse-power obtainable from one miner’s inch of water.
“The power necessary for different mill parts is:
For each 850 lb. stamp, dropping 6 inches 95 times per minute, 1·33 h.p. For each 750 lb. stamp, dropping 6 inches 95 times per minute, 1·18 h.p. For each 650 lb. stamp, dropping 6 inches 95 times per minute, 1·00 h.p. For an 8-inch by 10-inch Blake pattern rock-breaker 9·00 h.p. For a Frue or Triumph vanner, with 220 revolutions per minute 0·50 h.p. For a 4-feet clean-up pan, making 30 revolutions per minute 1·50 h.p. For an amalgamating barrel, making 30 revolutions per minute 2·50 h.p. For a mechanical batea, making 30 revolutions per minute 1·00 h.p.
The writer has had small practical experience of the working of that excellent hydraulic motor, the Pelton wheel, but if by horse-power in the table given is meant nominal horse-power, it appears to be high. Working with 800 cwt. stamps, 80 blows a minute, 1 h.-p. nominal per stamp will be found sufficient with any good modern engine, which has no further burden than raising the stamps and pumping the feed water. It is always well, however, particularly when providing engine power, to err on the right side, and make provision for more than is absolutely needed for actual battery requirements. This rule applies with equal potency to pumping engines.
TO AVOID LOSS IN CLEANING UP.
The following, is a hint to quartz mill managers with respect to that common source of loss of gold involved in the almost inevitable loss of mercury in cleaning up operations. I have known hundreds of pounds’ worth of gold to be recovered from an old quartz mill site by the simple process of washing up the ground under the floor.
If you cannot afford to floor the whole of the battery with smooth concrete, at all events smoothly concrete the floor of the cleaning-up room, and let the floor slope towards the centre: where a sink is provided. Any lost mercury must thus find its way to the centre, where it will collect and can be panned off from time to time. Of course an underground drain and mercury trap must be provided.
IRON EXTRACTOR.
When using self-feeders, fragments of steel tools are especially liable to get into the battery boxes or other crushing appliance where they sometimes cause great mischief. I believe the following plan would be a practicable remedy for this evil.
By a belt from the cam or counter shaft, cause a powerful electric magnet to extract all magnetic particles; then, by a simple ratchet movement, at intervals withdraw the magnet and drop the adhering fragments into a receptacle by automatically switching off the electric current. A powerful ordinary horse-shoe magnet might probably do just as well, but would require to be re-magnetised from time to time.
TO SILVER COPPER PLATES.
To silver copper plates, that is, to amalgamate them on the face with mercury, is really a most simple operation, though many battery men make a great mystery of it. Indeed, when I first went into a quartz mill the process deemed necessary was not only a very tedious one, but very dirty also.
To amalgamate with silver, in fact, to silver-plate your copper without resort to the electro-plating bath, take any old silver (failing that, silver coin will do, but is more expensive), and dissolve it in somewhat dilute nitric acid, using only just sufficient acid as will effect the purpose. When the crystals have formed, add sufficient clean quick mercury to form a thick pasty amalgam; moderate heat will assist the process. After some hours place the ball of amalgam in a piece of strong new calico and squeeze out any surplus mercury.
About an ounce of silver to the foot of copper is sufficient. To apply it on new plates use somewhat dilute nitric acid applied with a swab to free the surface of the copper from oxides or impurities, then rub the ball of amalgam over the surface, using some little force. It is always well when copper-plates are coated with silver or zinc by means of mercury to let them stand dry for a day or two before using, as the mercury oxidises and the coating metal more closely adheres.
Only the very best copper-plate procurable should be used for battery tables; bad copper will always give trouble, both in the first “curing,” and after treatment. It should not be heavily rolled copper, as the more porous the metal the more easily will the mercury penetrate and amalgamate. I cannot agree that any good is attained by scouring the plates with sand and alkalies, as recommended in some books on the subject; on the contrary, I prefer the opposite mode of treatment, and either face the plates with nitrate of silver and nitrate of mercury, or else with sulphate of zinc and mercury, in the form of what is called zinc amalgam. If mine water, which often contains free sulphuric acid, is being used, the latter plan is preferable.
The copper should be placed smoothly on the wooden table and secured firmly thereto by copper tacks. If the plate should be bent or buckled, it may be flattened by beating it with a heavy hammer, taking care to interpose a piece of inch-thick soft wood between hammer and plate.
To coat with mercury only, procure some nitrate of mercury. This is easily made by placing mercury in a glazed earthenware bowl, pouring somewhat dilute nitric acid on it, and letting it stand till the metallic mercury is changed to a white crystal. Dense reddish-brown fumes will arise, which are injurious if breathed, so the operation should be conducted either in the open air, or where there is a draught.
Now have your silvering solution ready, which is to be somewhat diluted with water, next take two swabs, with handles about 12 inches long, dip the first into a basin containing dilute nitric acid, and rub it rapidly over about a foot of the surface of the plate; the oxide of copper will be absolutely removed, and the surface of the copper rendered pure and bright; then take the other swab, wet with the dilute nitrate of mercury, and pass it over the clean surface, rubbing it well in. Continue this till the whole plate has a coating of mercury. It may be well to go over it more than once. Then turn on the water and wash the plate clean, sprinkle with metallic mercury, rubbing it upwards until the plate will hold no more.
A basin with nitrate of mercury may be kept handy, and the plates touched up from time to time for a few days until they get amalgamated with gold, after which, unless you have much base metal to contend with, they will give no further trouble.
It must be remembered, however, that an excessive use of nitric acid will result in waste of mercury, which will be carried off in a milky stream with the water; and also that it will cause the amalgam to become very hard, and less active in attracting other particles of gold.
If you are treating the plate with nitrate of silver prepared as already mentioned, clean the plate with dilute nitric acid, rub the surface with the ball of amalgam, following with the swab and fairly rubbing in. It will be well to prepare the plate some days before requiring to use it, as a better adhesion of the silver and copper takes place than if mercury is applied at once.
To amalgamate with zinc amalgam, clean the copper plate by means of a swab, with fairly strong sulphuric acid diluted with water; then while wet apply the zinco-mercury amalgam and well rub in. To prepare the zinc amalgam, clip some zinc (the lining of packing cases will do) into small pieces and immerse them in mercury after washing them with a little weak sulphuric acid and water to remove any coating of oxide. When the mercury will absorb no more zinc, squeeze through chamois leather or calico (as for silver amalgam), and well rub in. The plate thus prepared should stand for a few days, dry, before using. If, before amalgamation with gold takes place, oxide of copper or other scum should rise on this plate a little very dilute sulphuric acid will instantly remove it.
Sodium and cyanide of potassium are frequently used in dressing-plates, but the former should be very sparingly employed, as it will often do more harm than good by taking up all sorts of base metals with the amalgam, and so presenting a surface which the gold will pass over without adhering to. Where water is scarce, and is consequently used over and over again, lime may be added to the pulp, or, if lime is not procurable, wood ashes may be used. The effect is two-fold; the lime not only tends to “sweeten” sulphide ores and keep the tables clean, but also causes the water to cleanse itself more quickly of the slimes, which will be more rapidly precipitated. When zinc amalgam is used, alkalies would, of course, be detrimental.
When no other water than that from the mine is available, difficulties often arise owing to the impurities it contains. These are various, but among the most common are the soluble sulphates, and sometimes free sulphuric acid evolved by the oxidisation of metallic sulphides. In the presence of this difficulty, do one of two things: either utilise or neutralise. In certain cases, I recommend the former. Some time since I was treating, for gold extraction, material from a mine which was very complex in character. For this ore I coined the term “polysynthetic.” This contained about half a dozen different sulphides. The upper parts of the lode being partially oxidised, free sulphuric acid (H₂SO₄) was evolved. I therefore, following out a former discovery, added a little metallic zinc to the mercury in the boxes and on the plates with excellent results. When the free acid in the ore began to give out in the lower levels I added minute quantities of sulphuric acid to the water from time to time. I have since found, however, that with some water, particularly West Australian, the reaction is so feeble (probably owing to the lime and magnesia present) as to make this mode of treatment unsuitable.
HOW TO MAKE A DOLLY.
I have seen some rather elaborate dollies, intended to be worked with amalgamating tables, but the usual prototype of the quartz mill is set up, more or less, as follows: A tree stump, from 9 in. to a foot diameter, is levelled off smoothly at about 2 ft. from the ground; on this is firmly fixed a circular plate of ½ in. iron, say 9 in. in diameter; a band of ³/₁₆ in. iron, about 8 or 9 in. in height, fits more or less closely round the plate (Fig. 35). This is the battery box. A beam of heavy wood, about 3 in. diameter and 6 ft. long, shod with iron, is vertically suspended, about 9 in. above the stump, from a flexible sapling with just sufficient spring in it to raise the pestle to the required height. About 2 ft. from the bottom the hanging beam is pierced with an auger hole and a rounded piece of wood, 1½ in. by 18 in., is driven through to serve as a handle for the man who is to do the pounding. His mate breaks the stone to about 2 in. gauge and feeds the box, lifting the ring from time to time to sweep off the triturated gangue, which he screens through a sieve into a pan and washes off, either by means of a cradle or simply by panning. In dollying it generally pays to burn the stone, as so much labour in crushing is thus saved. A couple of small kilns to hold about a ton each dug out of a clay bank will be found to save fuel where firewood is scarce, and will more thoroughly burn the stone and dissipate the base metals, but it must be remembered that gold from burnt stone is liable to become so encrusted with the base metal oxides as to be difficult to amalgamate. Fig. 35A represents another primitive dolly (Plate VI. hand dollying).