The exterior diameter of the circular iron belt must be precisely equal to that of the ring, because, if larger, the free movement of the rubbers to and fro on the concave refracting surface AC (fig. 110) could not take place.

By what is already said, it will be obvious that the grinding process is begun at the refracting sides AC and BC, and a few words will shew that this could hardly be otherwise. If a commencement be made on the reflecting side, which appears at first sight more natural, the consequence is obvious. Having provided for an excess of material in every direction, the segment must consequently be larger than it will be when finished; and the surfaces therefore cannot be true and perfect, except they be ground throughout their entire segmental section, from their centres of curvature, in reference to some given apex of the generating triangle. Now, if the reflecting side were finished first, it might continue to possess this excess of size after being finished, and would, therefore, afford no accurate starting point for the grinding of the other surfaces; it would also present no surface or narrow plane for resting firmly on the iron belt, but would then depend merely on its own finished plane, which, being curved and considerably inclined, would not give a solid bearing for the glass. The other mode of commencing with the two refracting sides, on the contrary, gives a solid bearing on the narrow plane already ground on the reflecting side at A; and after these surfaces have been ground, and the segments inverted (as shewn in fig. 111), the outer edge of this narrow plane at the arris A, which has been fully defined by the intersection of the finished surface AC just ground, and also the apex at C, which has been determined by the intersection of AC and BC, combine to fix an accurate starting point for the rubber, in grinding the reflecting surface AB.

Fig. 111.

Inverted ring segment

Dressing off the rough part of the Ring.

The ring is generally reduced from the rough state by means of fixed rubbers, the adjustment of which is more easily regulated than that of the moveable beam or radius of the arc, which is used to give the exact curvature of the surface. Those fixed rubbers are 150 millimètres (nearly 6 inches) wide, by 200 millimètres (nearly 8 inches) long, and are of cast-iron. Three such rubbers are placed at equidistant points of the circle. Two cutters of sheet-iron attached to arms placed vertically (as are also those which carry the rubbers), and moving in grooves radiating towards the centre of the lathe, so as to admit of adjustment to suit the varying radii of the zones, serve gradually to abrade the outer and inner arrises of the segments, so as to prevent the splintering to which, from becoming too sharp, those arrises, without this precaution, would be liable. Those rubbers are, besides, fixed by stems to frames, in the form of quadrants of the circle, which allow of a change in the direction of the planes, as occasion may require.

Instead of the siliceous sand formerly used, the powder of pounded freestone is employed, as it is found to wear the tools less, and to form a better preparation for the subsequent grinding operations. It is easy to conceive that the action of the fixed rubbers necessarily produces ruts or inequalities in the circular direction. The operation of rough dressing, therefore, is not finished until, when those first rubbers are removed, the surfaces of the segments have been subject, for the required time, to the action of moveable rubbers, attached to arms working as radii of curvature, in a plane at right angles to the horizontal movement of the lathe, which carries the zones.

The Emery Grinding.

The form of the segment should be nearly perfect, after the rough grinding is finished. The lathe and the zone are then subjected to an extremely careful washing. Every place where the stone-powder might adhere is dusted. The radius of curvature is verified afresh, agreeably to the co-ordinates (Appendix, No. IV.); and emery is used instead of powdered stone; beginning with that called No. 1, which is drawn after suspension in water for one minute. Brushes are used for spreading the emery on the surface of the glass. The quantity ought always to be sufficient to prevent the direct contact of the cast-iron rubber with the glass. Splintering or scratching, which cannot be easily effaced, may result from the neglect of this precaution.

Practice alone, and an eye duly trained by continual experience, can determine the point of time at which each kind of emery must be discontinued. The celerity of the work depends on circumstances very difficult to appreciate, such as the amount of the pressure of the rubbers, or the degree of accuracy with which the radius of curvature has been adjusted, during the rough grinding. Each kind of emery in succession thus corrects the form of the zone and refines the grain of the surface of the glass; and each change to a fresh material requires the same attention to cleanliness, so as to remove every trace of the substance last used in grinding, and thus to give each successive process its full and legitimate effect. The douci is the fifth and last kind of emery which precedes the polish. It is drawn off after ten minutes’ suspension in water, and is extremely fine. Before applying it, the greatest care is necessary to insure cleanliness, as a single grain of any of the preceding kinds of emery might cause scratches, which the polish cannot remove.

The Polish.

The same considerations which induce the workman most carefully to cleanse the lathe and everything connected with it, before employing the last emery called the douci, are still more urgent in the case of the final polish. The only change which is made at this last stage of the work is to replace the first rubber by a new one, both longer and wider by about 50 millimètres (nearly 2 inches). On its lower face is attached with cement a piece of soft carpet, whose edges are fixed to the rubber by means of flat bands of iron, attached with screws. This security, added to that given by the cement, is necessary to fit it to resist the great pressure it must sustain. A practical question, which experience alone can resolve, occurs at this stage, as the operation of polishing may, in the hands of unskilful persons, be so inopportunely commenced, as to make that work almost endless. Thus, the mere circumstance of spreading at the beginning too thick layers of rouge, or using unsuitable kinds of carpet, would cut scratches in the glass, and thus perhaps make it necessary to return to the use of the emery called douci. Sometimes, also, if the carpets be not washed at the very time of using them, scratches are formed by the dust which they may contain. This shews, that the use of rouge should be rather sparing than otherwise, at the commencement of the polish; and that the carpet-cloths should be brushed and washed twice rather than once. In all cases, the quality of the carpet forms an important element in the success of the working.

When the polish is finished, the ring is detached from the circular belt, simply by the tap of a hammer, on the inner edge of the circle. The division of the zones (which are quarters of the circle) into eighths, is done by means of a sawing machine consisting of a flat copper-wheel, one-half millimètre (¹⁄₅₀th inch) in thickness, attached to an arm with a counterpoise. This wheel descends and cuts the zone by means of emery, which is continually applied to it; the direction of the cut is radial. The two halves of the zone are detached from each other, as soon as their weight exceeds the resistance of the part which remains to be sawn.

Adjustment of the Prisms.

The adjustment of the prisms in the frames, involves an operation which is not without risk. Much care is required in handling the sharp arrises of the glass, which are very acute and delicate and at the same time lie in a curved direction, which makes them liable to be splintered in the hands of unskilful persons.

With the exception of the plane vertical surfaces of the annular lenses, and the central band and rings of the dioptric belts of fixed lights, which are ground by means of vertical rubbers with a reciprocating movement, every other plane surface is executed by hand on a flat table.

Composition of the Cement for fixing the glass on the lathe.

8parts Swedish pitch.
1do. of wood ashes.

The whole is heated in an iron pot until fully liquified and thoroughly mixed. This cement is used almost in a state of ebullition, so that it cannot be handled without the precaution of continually dipping the hands in cold water.

Composition of cement used for the adjustment of the pieces of glass which touch each other.

12partswhite lead.
1do.minium or red lead.
5do.boiled lintseed oil.

The whole is pounded on an iron table by means of a flat mullet, like that used by painters (fig. 112), whose grinding surface is a b, and c the knob for the hand. This cement is applied liquid so as to offer no resistance to the close union of the pieces, which it is intended to unite.

Fig. 112.

Painter's mullet

Cement for filling up voids, and fixing the rings in the frames.

12partswhite lead.
3do.whiting.
1do.minium.
4do.boiled lintseed oil.

This last composition differs from the former only in the introduction of whiting, which, while like minium it has a desiccative property, gives more body to the cement and prevents the formation of cracks. The oil is also decreased in quantity, as the cement must be used in a more compact state. The trituration of this cement is performed by means of a cylindric iron roller a b, with a centre-spoke c d for the hand (fig. 113).

Fig. 113.

Roller

It is essential for the production of good cement, that the mixture of the ingredients be complete.

Prices of the various parts of the Dioptric Apparatus.

The expense of the various parts of the Dioptric apparatus is as follows: Great lens of first order, L.58 (8 of which are required); pyramidal lens and mirror, L.14, 12s. (8 of which are required); catadioptric cupola, L.480; catadioptric rings below lenses, L.360; pannel of dioptric belt for fixed light of first order, L.56 (of which 8 are required for the whole circle); apparatus of fourth order, for a fixed light, for whole horizon, L.128; apparatus of sixth order, for whole horizon, L.44. The expense of the mechanical lamp of the first order with four wicks, as made for the Scotch Lighthouses by Mr John Milne of Edinburgh, is L.30.

Diagrams illustrative of the Table, Appendix, No. IV.

Fig. 114.

References to table