The Invention of Lithography
From this book
| (3) | Wax | 4 | parts |
| Spermaceti | 4 | parts | |
| Soap | 4 | parts | |
| Lampblack | 2 | parts |
The first three materials are melted together, the lampblack is added, and then the whole is treated as before.
| (4) | Wax | 8 | parts |
| Spermaceti | 4 | parts | |
| Soap | 4 | parts | |
| Lampblack | 2 | parts |
The wax is to be half burned away, then the spermaceti and soap are to be melted into it, and the whole treated as the other formulas.
| (5) | Shellac | 4 | parts |
| Wax | 8 | parts | |
| Soap | 5 | parts | |
| Lampblack | 3 | parts |
The shellac is to be completely dissolved with the wax by means of combustion after which the rest of the treatment is the same as before.
| (6) | Shellac | 4 | parts |
| Wax | 8 | parts | |
| Tallow | 2 | parts | |
| Soap | 5 | parts | |
| Lampblack | 3 | parts |
The same treatment, except that the tallow is to be mixed in after the shellac has dissolved. This crayon is a little softer than the others. The same is true of the following two.
| (7) | Wax | 8 | parts |
| Tallow | 4 | parts | |
| Soap | 6 | parts | |
| Lampblack | 3 | parts |
Wax, tallow, and soap are melted together and burned till one third of the mass has been consumed. Then the lampblack is added and the rest of the process is as before.
| (8) | Wax | 2 | parts |
| Tallow | 6 | parts | |
| Mennig | 2 | parts | |
| Lampblack | 2 | parts |
Wax, mennig, and lampblack are heated and constantly stirred till the mennig dissolves in froth and changes from red to brown. Then the lampblack is rubbed in thoroughly, the whole warmed again properly and shaped into sticks.
These are the best compositions, thoroughly tested by me, and it is very good to make a stock of all or most of them. In the case of the recipes for chemical ink, the differences are not great, and it is largely a matter of taste as to which kind one may use. But in the case of the crayons, each of them produces a different grain which creates a particular effect; so that by using various kinds of crayon one will gain greater perfection of work, or, at least, find execution easier than with only one crayon. Also, they are in proportion to the greater or lesser roughness of the stones; and the darker shadings are easier to produce with soft crayons than with hard ones, while the hard ones are best for fine shading and outlines.
The lampblack used for crayons must be burned out first, else it will develop blisters, which is the case also if the composition is poured on the plates too hot.
Crayon that contains much shellac is likely to soften in damp air; therefore it should be kept in tightly closed vessels.
IX CONCERNING COLOR FOR PRINTING
The manufacture of printing-ink or color is very difficult and dangerous on a large scale. I counsel all to take lessons from a book printer when he makes it.
The varnish must be prepared in the open, far from buildings, because of its combustibility. The best utensils and skilled workmen are required, because otherwise terrible accidents may occur, and even life be lost through explosion of the copper receptacle. Whoever does not require as much as one or more hundredweight of varnish in a year, would better buy it from printers or make only a small quantity, one or two pounds, and in an open vessel. For this purpose I will describe the process.
One, or at most two pounds of good old but not rancid linseed oil are poured into a clean iron pan which has a long, strong handle and is so large that the oil takes up only one half or, better, one third of the space. This is heated over a good fire till it burns, which is facilitated by applying flame to it. Oil that is too new has much water and other impurities that make it froth and run over. In that case the oil must be poured into the pan only in small quantities, when one must take great care to avoid spattering. As soon as the oil burns, the pan is removed from the fire and placed in a safe spot. If it is hot enough, it will continue to burn. It must now be stirred from time to time with an iron rod. Usually the flame increases under this stirring, but sinks again immediately at its cessation. So long as it does this, there is no danger that the flame cannot be easily extinguished if need be. But when it begins to continue burning with a great flame after the stirring stops, and at the same time to bubble and froth, it is high time to cover the pan with a close lid and leave it covered till the oil no longer takes fire when exposed again to the air. Then a dry knife is introduced and as much oil removed as will adhere to its point. If it does not permit itself to be pulled into long threads when cool, but is too thin, it must be heated again until it gets the required consistency.
A good varnish dries very readily of itself, and it is not only unnecessary but inadvisable to mix a drier with it, as varnish so treated is too likely to off-set on the stone.
Several strengths of printing-varnish are needed for the various methods of lithography. Therefore a stock of thin, medium, and thick varnish is needed.
In making the thin, the oil has been reduced to about two thirds through combustion. It is somewhat like fluid honey and does not pull into threads.
Only a little more than half the oil is left in the case of medium varnish. It is thick as old honey and can be pulled into threads a foot long.
In the thick varnish the mass is not much less, but it can be pulled into threads of a yard in length; and further boiling makes it thick and tough like gum elastic. In the latter case it can be used with advantage when rubbed down with oil and properly thinned. But as soon as it has obtained the last-mentioned degree of thickness and toughness, it must be cooled quickly, for then it is not far from hardening completely and becoming worthless. In the beginning it requires a long while for the oil to reach the first degree of thickness, an hour or more for a pound. But after that period the thickening progresses rapidly, so that a quarter of the time will bring it to the point of total toughness.
To make printing color of the varnish, the proper amount of lampblack must be mixed in. The roasted or burned-out is best in this also, because the ordinary lampblack delays the drying and turns yellow with time.
The more lampblack is mixed in, and the more thoroughly they are combined by rubbing down, the better will be the color. But lampblack must not be added in such quantities that the color becomes dough-like.
In describing the various styles of printing I will describe the best printing-inks also. I will merely make the general note here that designs on stone take the ink best when it is thin and fluid, but that there is less danger of off-set on the parts of the stone that are to remain white, if the ink is tougher or contains more lampblack.
Too much lampblack and too tough a varnish endanger the finer strokes and dots, however, so that they will not take ink, being, as lithographers say, rubbed out. The rubbing or grinding effect of too tough an ink is like that of pumice or other grinding material. With tougher varnish, clearer imprints can be made and they do not become yellow easily. But the inking is more difficult and demands greater skill, as well as heavier pressure in the press.
The varnish can be mixed not only with lampblack but with many other colors, which will be described when I reach color printing in this essay. Sometimes black lacquer is used with advantage instead of lampblack; and Frankfurter black is successful in the intaglio and aquatint methods.
X RUBBING-UP INK
It happens often that weak parts of a design cannot withstand the etching fluid and are cut away; also, that fine lines are rubbed away through unskilled treatment during printing. Then frequently a very simple remedy is to ink the plate with the so-called rubbing-up ink.
This color consists of a thin varnish in which a portion of litharge of silver or mennig or white lead has been dissolved thoroughly over the fire, and a proper amount of lampblack added. Often it is good to add some finely powdered sand or powdered pumice stone.
To prepare this, a portion of the thinnest varnish is heated in a pan till it burns. Then about an ounce of finely powdered mennig (or another lead oxide) is stirred in to each sixteen ounces of varnish till all is thoroughly mixed.
A rubbing-up ink can be made also by mixing common printer's ink with vegetable oil, tallow, and a very little soap.
Each of these colors adheres to all those places that have a trace of fat and thus gradually makes faint places in a design receptive again.
Later I will describe how to use care in applying this color, so that the entire stone shall not be smutted and spoiled.
CHAPTER III CONCERNING ACIDS AND OTHER MATERIALS
I GENERAL PROPERTIES OF ACIDS
Probably most lithographers still believe, as I did once, that the etching with acids prepares the stone, and that the succeeding application of gum merely increases this preparation. Countless experiments have taught me that the exact reverse is true. Gum arabic and a few other similar bodies are the true factors in preparation, and the acids simply make the stone more receptive for them. Only sulphuric acid, which changes the surface of the stone into gypsum, prepares it without gum; but this is available only for a few intaglio methods.
The stone used for lithography consists mostly of limestone sated with carbonic acid. Most acids, and even the salts, possess more affinity for limestone than the carbonic acid, which latter is freed and escapes in gaseous form as soon as another acid touches the stone. If aquafortis, muriatic acid, vinegar, etc., is poured on the stone, there rise a number of air blisters, which are nothing except the escaping carbonic acid, and the applied fluid seems to boil, in degree according to its strength. The boiling and bubbling last till the fluid has sated itself with lime, after which it becomes still, and is impotent for further etching.
The direct effect is the solution and destruction of parts of the surface of the stone. If it has been coated in parts with a fatty substance that resists the etching fluid, the places so coated are left untouched, so that, when the stone is cleaned, all the fat-coated lines and dots are in relief.
If the stone is coated with fatty matter, but not so thickly that the acid is entirely resisted, it will pierce the covering and eat away more or less of the stone. If the etching is continued or if the acid is strong, the fatty coat will be destroyed entirely, the surface of the stone will be clean, and ready for the ensuing preparation. The preparation of the stone for pen drawings with oil or soap-water and several aquatint methods, is based on this principle, that a very thin coating of grease can be etched away partly or wholly, at will.
After eating away the surface of the stone the acids have the property of giving it a fine polish.
Therefore if the stone has been covered with a design, and then etched with an acid, it could be inked and printed many times, as long as it is kept properly dampened and not too much pressure is used in applying the ink. However, this could be done also with a thoroughly clean stone, using only water, though the polish obtained from etching makes it much easier. But this apparent preparation is not by any means sufficient to print with certainty; and it becomes perfect only if the stone is coated with a solution of gum arabic in water after being etched. If a plate that has been merely etched and not treated with gum becomes dry during printing, or even if too much pressure be used in applying ink or in cleaning with the more or less smutty cleaning rags, it generally takes color and smut which are extremely hard to remove.