Fig. 11.—Sectional diagram illustrating waste of glass in grinding curved or irregular plate.

While it is evident that careful design of the rolling table will avoid all tendency to the formation of sheets of such undesirable form, it is a much more difficult matter to avoid all distortion of the sheet during the annealing process and while the sheet is being moved from the rolling table to the annealing kiln. Owing to the great size of the slabs of glass to be dealt with, and still more to the stringent requirement of flatness, the continuous annealing kiln, in which the glass travels slowly down a tunnel from the hot to the cold end, has not been adopted for the annealing of plate-glass, and a form of annealing kiln is still used for that glass which is similar in its mode of operation to the old-fashioned kilns that were used for other kinds of glass before the continuous kiln was introduced. These kilns simply consist of chambers in which the hot glass is sealed up and allowed to cool slowly and uniformly during a more or less protracted period. In the case of plate-glass, the slabs are laid flat on the stone bed of the kiln. This stone bed is built up of carefully dressed stone, or blocks of fire-brick bedded in sand in such a way that they can expand freely laterally without causing any tendency for the floor to buckle upwards as it would do if the blocks were set firmly against one another. The whole chamber is previously heated to the requisite temperature at which the glass still shows a very slight plasticity. The hot glass slabs from the rolling table are laid upon the bed of this kiln, several being usually placed side by side in the one chamber, and the slabs in the course of the first few hours settle down to the contour of the bed of the kiln, from which shape and position they are never disturbed until they are removed when quite cold. In modern practice the cooling of a kiln is allowed to occupy from four to five days; even this rate of cooling is only permissible if care is taken to provide for the even cooling of all parts of the kiln, and for this purpose special air-passages are built into the walls of the chamber and beneath the bed upon which the glass rests, and air circulation is admitted to these in such a way as to allow the whole of the kiln to cool down at the same rate; in the absence of such special arrangements, the upper parts of the kiln would probably cool much more rapidly than the base, so that the glass would be much warmer on its under than on its upper surface.

When the slabs of plate-glass are removed from the annealing kilns they very closely resemble sheets of rolled plate in appearance, and they are quite sufficiently transparent to allow of examination and the rejection of the more grossly defective portions; the more minute defects, of course, can only be detected after the sheets have been polished, but this preliminary examination saves the laborious polishing of much useless glass.

The process of grinding and polishing plate-glass consists of three principal stages. In the first stage the surfaces of the glass are ground so as to be as perfectly flat and parallel as possible; in order to effect this object as rapidly as possible, a coarse abrasive is used which leaves the glass with a rough grey surface. In the second stage, that of smoothing, these rough grey surfaces are ground down with several grades of successively finer abrasive until finally an exceedingly smooth grey surface is left. In the third and final stage, the smooth grey surface is converted into the brilliant polished surface with which we are familiar by the action of a polishing medium.

Originally the various stages of the grinding and polishing processes were carried out by hand, but a whole series of ingenious machines has been produced for effecting the same purpose more rapidly and more perfectly than hand-labour could ever do. We cannot hope to give any detailed account of the various systems of grinding and polishing machines which are even now in use, but must content ourselves with a survey of some of the more important considerations governing the design and construction of such machinery.

In the first place, before vigorous mechanical work can be applied to the surface of a plate of glass, that plate must be firmly fixed in a definite position relatively to the rest of the machinery, and such firm fixing of a plate of glass is by no means readily attained, since the plate must be supported over its whole area if local fracture is to be avoided. While the surface of the plate is in the uneven condition in which it leaves the rolling table, such a firm setting of the glass can only be attained by bedding it in plaster, and this must be done in such a manner as to avoid the formation of air-bubbles between plaster and glass; if bubbles are allowed to form, they constitute places where the glass is unsupported. During the grinding and polishing processes these unsupported places yield to the heavy pressure that comes upon them, and irregularities in the finished polished surfaces result. The most perfect adhesion between glass and plaster is attained by spreading the paste of plaster on the up-turned surface of the slab of glass and lowering the iron bed-plate of the grinding table down upon it, the bed-plate with the adhering slab of glass being afterwards turned over and brought into position in the grinding machine. When one side of the glass has been polished, it is generally found sufficient to lay the slab down on a bed of damp cloth, to which it adheres very firmly, although sliding is entirely prevented by a few blocks fixed to the table in such a way as to abut against the edges of the sheet. In many works, however, the glass is set in plaster for the grinding and polishing of the second side as well as of the first.

The process of grinding and polishing is still regarded in many plate-glass works as consisting of three distinct processes, known as rough grinding, smoothing and polishing respectively. Formerly these three stages of the process were carried out separately; at first by hand, and later by three different machines. In the most modern practice, however, the rough and smooth grinding are done on the same machine, the only change required being the substitution of a finer grade of abrasive at each step for the coarser grade used in the previous stage. For the polishing process, however, the rubbing implements themselves must be of a different kind, for while the grinding and smoothing is generally done by means of cast-iron rubbers moving over the glass, the polishing is done with felt pads. The table of the machine, to which the glass under treatment is attached, is therefore made movable, and when the grinding and smoothing processes are complete, the table with its attached glass is moved so as to come beneath a superstructure carrying the polishing rubbers, and the whole is then elevated so as to allow the rubbers to bear on the glass.

The earliest forms of grinding machines gave a reciprocal motion to the table which carries the glass, or the grinding rubbers were moved backward and forward over the stationary table. Rotary machines, however, were introduced and rapidly asserted their superiority, until, at the present time, practically all plate-glass is ground on rotating tables, some of these attaining a diameter of over 30 ft. The grinding “rubbers” consist of heavy iron slabs, or of wood boxes shod with iron, but of much smaller diameter than the grinding table. The rubbers themselves are rotary, being caused to rotate either by the frictional drive of the rotating table below them, or by the action of independent driving mechanism, but the design of the motions must be so arranged that the relative motion of rubber and glass shall be approximately the same at all parts of the glass sheets, otherwise curved instead of plane surfaces would be formed. This condition can be met by placing the axes of the rubbers at suitable points on the diameter of the table. The abrasive is fed on to the glass in the form of a thin paste, and when each grade or “course” has done the work required of it, the whole table is washed down thoroughly with water and then the next finer grade is applied. The function of the first or coarsest grade is simply to remove the surface irregularities and to form a rough but plane surface. The abrasive ordinarily employed is sharp sand, but only comparatively light pressure can be applied, especially at the beginning of this stage, since at that period the weight of the rubber is at times borne by relatively small areas of glass that project here and there above the general level of the slab. As these are ground away, the rubbers take a larger and more uniform bearing, and greater pressure can be applied. The subsequent courses of finer abrasives are only required to remove the coarse pittings left in the surface by the action of the first rough grinding sand; the finer abrasive replaces the deep pits of the former grade by shallower pits, and this is carried on in a number of steps until a very smooth “grey” surface is attained and the smoothing process is complete. The revolving table or “platform” is now detached from the driving mechanism, and moved along suitably placed rails on wheels provided for that purpose, until it stands below the polishing mechanism. Here it is attached to a fresh driving mechanism, and it is then either raised so as to bring the glass into contact with the felt-covered polishing rubbers, or the latter are lowered down upon the glass. The polishing rubbers are large felt-covered slabs of wood or iron which are pressed against the glass with considerable force; their movement is very similar to that of the grinding rubbers, but in place of an abrasive they are supplied with a thin paste of rouge and water. The time required for the polishing process depends upon the perfection of the smoothing that has been attained; in favourable cases two or three hours are sufficient to convert the “grey” surface into a perfectly polished one; where, however, somewhat deeper pits have been left in the glass, the time required for polishing may be much longer, and the polish attained will not be so perfect. The mode of action of a polishing medium such as rouge is now recognised to be totally different in character from that of even the finest abrasive; the grains of the abrasive act by their hardness and the sharpness of their edges, chipping away tiny particles of the glass, so that the glass steadily loses weight during the grinding and smoothing processes. During the polishing process, however, there is little or no further loss of weight, the glass forming the hills or highest parts of the minutely pitted surface being dragged or smeared over the surface in such a way as to gradually fill up the pits and hollows. The part played by the polishing medium is probably partly chemical and partly physical, but it results, together with the pressure of the rubber, in giving to the surface molecules of the glass a certain amount of freedom of movement, similar to that of the molecules of a viscid liquid; the surface layers of glass are thus enabled to “flow” under the action of the polisher and to smooth out the surface to the beautiful level smoothness which is so characteristic of the surfaces of liquids at rest. This explanation of the polishing process enables us to understand why the proper consistency of the polishing paste, as well as the proper adjustment of the speed and pressure of the rubbers, plays such an important part in successful polishing; it also serves to explain the well-known fact that rapid polishing only takes place when the glass surface has begun to be perceptibly heated by the friction spent upon it.

Continue reading
Page 19 of 37