“The second point is the cause of the decay. An extensive series of experiments was carried out with a view of determining the causes of the decay of bindings. The sub-committee find that this is caused by both mechanical and by chemical influences. Of the latter, some are due to mistakes of the leather manufacturer and the bookbinder, others to the want of ventilation, and to improper heating and lighting of libraries. In some cases inferior leathers are finished (by methods in themselves injurious) so as to imitate the better class leathers, and of course where these are used durability cannot be expected. But in the main the injury for which the manufacturer and bookbinder are responsible must be attributed rather to ignorance of the effect of the means employed to give the leather the outward qualities required for binding, than to the intentional production of an inferior article.... Leathers produced by different tanning materials, although they may be equally sound and durable mechanically, vary very much in their resistance to other influences, such as light, heat, and gas fumes.
“For bookbinding purposes, the sub-committee generally condemn the use of tanning materials belonging to the catechol group, although the leathers produced by the use of these materials are for many purposes excellent, and indeed superior. The class of tanning materials which produce the most suitable leather for this particular purpose belong to the pyrogallol group, of which a well known and important example is sumach. East Indian or ‘Persian’ tanned sheep and goat skins, which are suitable for many purposes, and are now used largely for cheap bookbinding purposes, are considered extremely bad. Books bound in these materials have been found to show signs of decay in less than twelve months, and the sub-committee are inclined to believe that no book bound in these leathers, exposed on a shelf to sunlight or gas fumes, can ever be expected to last more than five or six years. Embossing leather under heavy pressure to imitate a grain has a very injurious effect, while the shaving of thick skins greatly reduces the strength of the leather by cutting away the tough fibres of the inner part of the skin. The use of mineral acids in brightening the colour of leather, and in the process of dyeing, has a serious effect in lessening its resistance to decay. A good deal yet remains to be learned about the relative permanency of the different dyes.”
On analysis free sulphuric acid was found to be present in nearly all bookbinding leather, and it is the opinion of the committee that even a small quantity of this acid materially lessens the durability of the leather.
“It has been shown by careful experiment, that even a minute quantity of sulphuric acid used in the dye bath to liberate the colour is at once absorbed by the leather, and that no amount of subsequent washing will remove it. In a very large proportion of cases the decay of modern sumach-tanned leather has been due to the sulphuric acid used in the dye bath, and retained in the skin. We have examined very many samples of leather manufactured and sold specially for bookbinding purposes, from different factories, bought from different dealers, or kindly supplied by bookbinders and by librarians, and have found them to contain, in a large number of cases, free sulphuric acid, from 0.5 up to 1.6 per cent.”
The publication of the report should tend to fix a standard for bookbinding leather. Hitherto there has been no recognised standard. Bookbinders have selected leather almost entirely by its appearance. It has now been shown that appearance is no test of durability, and the mechanical test of tearing the leather is insufficient. Sound leather should tear with difficulty, and the torn edges should be fringed with long, silky fibres, and any leather which tears very easily, and shows short, curled-up fibres at the torn edges, should be discarded. But though good bookbinding leather will tear with difficulty, and show long fibres where torn, that is in itself not a sufficient test; because it has been shown that the leather that is mechanically the strongest, is not necessarily the most durable and the best able to resist the adverse influences to which books are subject in libraries.
The report shows that bookbinders and librarians are not, as a general rule, qualified to select leather for bookbinding. In the old days, when the manufacture of leather was comparatively simple, a bookbinder might reasonably be expected to know enough of the processes employed to be able to select his leather. But now so complicated is the manufacture, and so many are the factors to be considered, that an expert should be employed.
“The committee have satisfied themselves that it is possible to test any leather in such a way as to guarantee its suitability for bookbinding. They have not come to any decision as to the desirability of establishing any formal or official standard, though they consider that this is a point which well deserves future consideration.”
It is to be hoped that some system of examining and hall-marking leather by some recognised body, may be instituted. If librarians will specify that the leather to be employed must be certified to be manufactured according to the recommendations of the Society of Arts Committee, there is no reason why leathers should not be obtained as durable as any ever produced. This would necessitate the examining and testing of batches of leather by experts. At present this can be done more or less privately at various places, such as the Yorkshire College, Leeds, or the Herolds’ Institute, Bermondsey. In the near future it is to be hoped that some recognised public body, such as one of the great City Companies interested in leather, may be induced to establish a standard, and to test such leathers as are submitted to them, hall-marking those that come up to the standard. This would enable bookbinders and librarians, in ordering leather, to be sure that it had not been injured in its manufacture. The testing, if done by batches, should not add greatly to the cost of the leather.
On the question of the qualities of an ideal bookbinding leather the committee report:—
“It is the opinion of the committee, that the ideal bookbinding leather must have, and retain, great flexibility.... (It) must have a firm grain surface, not easily damaged by friction, and should not be artificially grained.... The committee is of opinion that a pure sumach tannage will answer all these conditions, and that leather can, and will, be now produced that will prove to be as durable as any made in the past.”
The committee has so far only dealt with vegetable-tanned leather. I have used, with some success, chrome-tanned calfskin. Chrome leather is difficult to pare, and to work, as it does not become soft when wet, like vegetable-tanned leather. It will stand any reasonable degree of heat, and so might perhaps be useful for top-shelf bindings and for shelf edging. It is extremely strong mechanically, but without further tests I cannot positively recommend it except for trial.
While the strength and probable durability of leather can only be judged by a trained leather chemist, there remains for the binders selection, the kind of leather to use, and its colour.
Most of the leather prepared for bookbinding is too highly finished. The finishing processes add a good deal to the cost of the leather, and are apt to be injurious to it, and as much of the high finish is lost in covering, it would be better for the bookbinder to get rougher leather and finish it himself when it is on the book.
The leathers in common use for bookbinding are:—
- Goatskin, known as morocco.
- Calf, known as calf and russia.
- Sheepskin, known as roan, basil, skiver, &c.
- Pigskin, known as pigskin.
- Sealskin, known as seal.
Morocco is probably the best leather for extra binding if properly prepared, but experiment has shown that the expensive Levant moroccos are nearly always ruined in their manufacture. A great many samples of the most expensive Levant morocco were tested, with the result that they were all found to contain free sulphuric acid.
Calf.—Modern vegetable-tanned calf has become a highly unsatisfactory material, and until some radical changes are made in the methods of manufacturing it, it should not be used for bookbinding.
Sheepskin.—A properly tanned sheepskin makes a very durable, though rather soft and woolly, leather. Much of the bookbinding leather now made from sheepskin is quite worthless. Bookbinders should refuse to have anything to do with any leather that has been artificially grained, as the process is apt to be highly injurious to the skin.
Pigskin.—Pigskin is a thoroughly good leather naturally, and very strong, especially the alumed skins; but many of the dyed pigskins are found to be improperly tanned and dyed, and worthless for bookbinding.
Sealskin is highly recommended by one eminent librarian, but I have not yet had any experience of its use for bookbinding.
The leather that I have found most useful is the Niger goatskin, brought from Africa by the Royal Niger Company; it is a very beautiful colour and texture, and has stood all the tests tried, without serious deterioration. The difficulty with this leather is that, being a native production, it is somewhat carelessly prepared, and is much spoiled by flaws and stains on the surface, and many skins are quite worthless. It is to be hoped that before long some of the manufacturers interested will produce skins as good in quality and colour as the best Niger morocco, and with fewer flaws.
Much leather is ruined in order to obtain an absolutely even colour. A slight unevenness of colours is very pleasing, and should rather be encouraged than objected to. That the want of interest in absolutely flat colours has been felt, is shown by the frequency with which the binders get rid of flat, even colours by sprinkling and marbling.
On this point I may quote from the committee: “The sprinkling of leather, either for the production of ‘sprinkled’ calf or ‘tree’ calf, with ferrous sulphate (green vitriol) must be most strongly condemned, as the iron combines with and destroys the tan in the leather, and free sulphuric acid is liberated, which is still more destructive. Iron acetate or lactate is somewhat less objectionable, but probably the same effects may be obtained with aniline colours without risk to the leather.”
CHAPTER XX
Paper—Pastes—Glue
PAPER
Paper may be made by hand or machinery, and either “laid” or “wove.” “Laid” papers are distinguished by wire marks, which are absent in “wove” paper.
A sheet of hand-made paper has all round it a rough uneven edge called the “deckle,” that is a necessary result of its method of manufacture. The early printers looked upon this ragged edge as a defect, and almost invariably trimmed most of it off before putting books into permanent bindings. Book-lovers quite rightly like to find traces of the “deckle” edge, as evidence that a volume has not been unduly reduced by the binder. But it has now become the fashion to admire the “deckle” for its own sake, and to leave books on hand-made paper absolutely untrimmed, with ragged edges that collect the dirt, are unsightly, and troublesome to turn over. So far has this craze gone, that machine-made paper is often put through an extra process to give it a sham deckle edge.
Roughly speaking, paper varies in quality according to the proportion of fibrous material, such as rag, used in the manufacture. To make paper satisfactorily by hand, a large proportion of such fibrous material is necessary, so that the fact that the paper is hand-made is to some extent a guarantee of its quality. There are various qualities of hand-made paper, made from different materials, chiefly linen and cotton rags. The best paper is made from pure linen rag, and poorer hand-made paper from cotton rag, while other qualities contain a mixture of the two or other substances.