And now, finally, let us say that you may do anything you can do in the painting of glass, so long as you do not lay the colour on too thick. The outline-touches should be flat upon the glass, and above all things should not be laid on so wet, or laid on so thick, that the pigment forms into a "drop" at the end of the touch; for this drop, and all pigment that is thick upon the glass like that, will "fry" when it is put into the kiln: that is to say, being so thick, and standing so far from the surface of the glass, it will fire separately from the glass itself and stand as a separate crust above it, and this will perish.

Plate IX. shows the appearance of the bubbles or blisters in a bit of work that has fried, as seen under a microscope of 20 diameters; and if you are inclined to disregard the danger of this defect as seen of its natural size, when it is a mere roughness on the glass, what do you think of it now? You can remove it at once by scraping it with a knife; and indeed, if through accident a touch here and there does fry, it is your only plan to so remove it. All you can scrape off should be scraped off and repainted every time the glass comes from the kiln; and that brings us to the important question of firing.


CHAPTER VII

Firing—Three Kinds of Kiln—Advantages and Disadvantages—The Gas-Kiln—Quick Firing—Danger—Sufficient Firing—Soft Pigments—Difference in Glasses—"Stale" Work—The Scientific Facts—How to Judge of Firing—Drawing the Kiln.

The way in which the painting is attached to the glass and made permanent is by firing it in a kiln at great heat, and thus fusing the two together.

Simple enough to say, but who is to describe in writing this process in all its forms? For there is, perhaps, nothing in the art of stained-glass on which there is greater diversity of opinion and diversity of practice than this matter of firing. But let us make a beginning by saying that there are, it may be said, three chief modifications of the process.

First, the use of the old, closed, coke or turf kiln.

Second, of the closed gas-kiln.

And third, of the open gas-kiln.

The first consists of a chamber of brick or terra-cotta, in which the glass is placed on a bed of powdered whitening, on iron plates, one above another like shelves, and the whole enclosed in a chamber where the heat is raised by a fire of coke or peat.

This, be it understood, is a slow method. The heat increases gradually, and applies to the glass what the kiln-man calls a "good, soaking heat." The meaning of this expression, of course, is that the gradual heat gives time for the glass and the pigment to fuse together in a natural way, more likely to be good and permanent in its results than a process which takes a twentieth part of the time and which therefore (it is assumed) must wrench the materials more harshly from their nature and state.

There are, it must be admitted, one or two things to be said for this view which require answering.

First, that this form of kiln has the virtue of being old; for in such a thing as this, beyond all manner of doubt, was fired all the splendid stained-glass of the Middle Ages.

Second, that by its use one is entirely preserved from the dangers attached to the misuse of the gas-kiln.

But the answers to these two things are—

First, that the method employed in the Middle Ages did not invariably ensure permanence. Any one who has studied stained-glass must be familiar with cases in which ancient work has faded or perished.

The second claim is answered by the fact, I think beyond dispute, that all objections to the use of the gas-kiln would be removed if it were used properly; it is not the use of it as a process which is in itself dangerous, but merely the misuse of it. People must be content with what is reasonable in the matter; and, knowing that the gas-kiln is spoken of as the "quick-firing" kiln, they must not insist on trying to fire too quick.

Now I have the highest authority (that of the makers of both kiln and pigment) to support my own conviction, founded on my own experience, in what I am here going to say.

Observe, then, that up to the point at which actual fusion commences—that is, when pigment and glass begin to get soft—there is no advantage in slowness, and therefore none in the use of fuel as against gas—no possible disadvantage as far as the work goes: only it is time wasted. But where people go wrong is in not observing the vital importance of proceeding gently when fusion does commence. For in the actual process of firing, when fusion is about to commence, it is indeed all-important to proceed gently; otherwise the work will "fry," and, in fact, it is in danger from a variety of causes. Make it, then, your practice to aim at twenty to twenty-five minutes, instead of ten or twelve, as the period during which the pigment is to be fired, and regulate the amount of heat you apply by that standard. The longer period of moderate heat means safety. The shorter period of great heat means danger, and rather more than danger.

Fig. 42 is the closed gas-kiln, where the glass is placed in an enclosed chamber; fig. 43 is the open gas-kiln, where the gas plays on the roof of the chamber in which the glass lies; fig. 44 shows this latter. But no written description or picture is really sufficient to make it safe for you to use these gas-kilns. You would be sure to have some serious accident, probably an explosion; and as it is absolutely necessary for you to have instruction, either from the maker or the experienced user of them, it is useless for me to tell lamely what they could show thoroughly. I shall therefore leave this essentially technical part of the subject, and, omitting these details, speak of the few principles which regulate the firing of glass.

FIG. 42.
Fig. 42.
FIG. 43.
Fig. 43.
FIG. 44.
Fig. 44.

And the first is to fire it enough. Whatever pigment you use, and with whatever flux, none will be permanent if the work is under-fired; indeed I believe that under-firing is far more the cause of stained-glass perishing than the use of untrustworthy pigment or flux; although it must always be borne in mind that the use of a soft pigment, which will "fire beautifully" at a low heat, with a fine gloss on the surface, is always to be avoided. The pigment is fused, no doubt; but is it united to the glass? What one would like to have would be a pigment whose own fusing-point was the same, or about the same, as that of the glass itself, so that the surface, at least, of the piece of glass softens to receive it and lets it right down into itself. You should never be satisfied with the firing of your glass unless it presents two qualifications: first, that the surface of the glass has melted and begun to run together; and second, that the fused pigment is quite glossy and shiny, not the least dull or rusty looking, when the glass is cool.

"What one would like to have."

And can you not get it?

Well, yes! but you want experience and constant watchfulness—in short, "rule of thumb." For every different glass differs in hardness, and you never know, except by memory and constant handling of the stuff, exactly what your materials are going to do in the kiln; for as to standardising, so as to get the glass into any known relation with the pigment in the matter of fusing, the thing has never, as far as I know, been attempted. It probably could not be done with regard to all, or even many, glasses—nor need it; though perhaps it might be well if a nearer approach to it could be achieved with regard to the manufacture of the lighter tinted glasses, the "whites" especially, on which the heads and hands are painted, and where consequently it is of such vital importance that the painting should have careful justice done to it, and not lose in the firing through uncertainty with regard to conditions.

Nevertheless, if you observe the rule to fire sufficiently, the worst that can happen is a disappointment to yourself from the painting having to an unnecessary extent "fired away" in the kiln. You must be patient, and give it a second painting; and as to the "rule of thumb," it is surprising how one gets to know, by constant handling the stuff, how the various glasses are going to behave in the fire. It was the method of the Middle Ages which we are so apt to praise, and there is much to be said for practical, craftsmanly experience, especially in the arts, as against a system of formulas based on scientific knowledge. It would be a pity indeed to get rid of the accidental and all the delight which it brings, and we must take it with its good and bad.

The second rule with regard to the question of firing is to take care that the work is not "stale" when it goes into the kiln. Every one will tell you a different tale about many points connected with glass, just as doctors disagree in every affair of life. In talking over this matter of keeping the colour fresh—even talking it over with one's practical and experienced friends generally—one will sometimes hear the remark that "they don't see that delay can do it much harm;" and when one asks, "Can it do it any good?" the reply will be, "Well, probably it would be as well to fire it soon;" or in the case of mixing, "To use it fresh." Now, if it would be "as well"—which really means "on the safe side"—then that seems a sufficient reason for any reasonable man.

But indeed I have always found it one of the chiefest difficulties with pupils to get them to take the most reasonable precautions to make quite sure of anything. It is just the same with matters of measurement, although upon these such vital issues depend. How weary one gets of the phrase "it's not far out"—the obvious comment of a reasonable man upon such a remark, of course, being that if it is out at all it's, at any rate, too far out. A French assistant that I had once used always to complain of my demanding (as he expressed it) such "rigorous accuracy." But there are only two ways—to be accurate or inaccurate; and if the former is possible, there is no excuse for the latter.

But as to this question of freshness of colour, which is of such paramount importance, I may quote the same authority I used before—that of the maker of the colour—to back my own experience and previous conviction on the point, which certainly is that fresh colour, used the same day it is ground and fired the same day it is used, fires better and fires away less than any other.

Continue reading